How to Diagnose Sink Marks on Injection Molded Parts — and Fix Them in the Right Order

Flat illustration of an injection molded enclosure cover with a shallow sink mark on its visible face above a rib, beside a cross-section showing the thick rib junction underneath

Your production samples arrive, and the part measures to print — but the visible face has a shallow dip, where a rib sits on the back. The supplier calls it cosmetic. Your customer calls it a reject. A sink mark is the most common cosmetic defect in injection molding, and one of the most misdiagnosed: the fix depends on where the mark sits, and the most expensive mistake is changing the process when the geometry is the problem.

A sink mark is a shallow depression where a thick section — a rib, a boss, or a wall junction — cooled and shrank after the surface had frozen, pulling the skin inward. Read the mark’s location: opposite a rib means the rib is too thick, near the gate means packing stopped too early, across a face means the wall is uneven. Fix in this order — geometry, then mold, then process — because no pack pressure can feed a section whose gate has frozen. A rib over 60% of the wall is the usual culprit; bring it to 50% and the marks disappear.

What a Sink Mark Is — and What It Is Not

When molten plastic fills a mold, it does not freeze all at once. The plastic touching the cold steel wall forms a solid skin within a fraction of a second, while the core of a thick section stays molten for much longer. As that core finally cools, it shrinks — all resins shrink as they cool — and because the skin has already set, the shrinking core has nowhere to take material from. So it pulls the skin inward. The result is a shallow, dish-shaped dip on the surface, always directly above the thick feature underneath.

Three distinctions matter, because each points to a different fix. A sink mark is a surface depression: the skin gave way. A void is the same shrinkage hidden inside the part: the skin was stiff enough to hold its shape — common in rigid resins such as unfilled polycarbonate or acrylic — so the core tore away from itself instead, leaving an internal bubble you may only find by sectioning the part or by X-ray. A sink mark is not a short shot (the cavity never filled, so the part is incomplete) and it is not a weld line (two flow fronts met and left a visible seam). If the surface is complete and the dimensions are right but there is a dip, it is a sink mark.

It is also worth stating plainly what a sink mark is not: a dimensional failure. The part still measures to print. That is exactly why sink marks cause so many arguments between buyers and suppliers. The supplier’s inspection sheet says the part passes; the buyer’s customer sees a dip in the middle of a gloss black cover and sends it back. The defect is cosmetic, but "cosmetic" does not mean unimportant — on a visible face, a sink mark reads as poor quality, it catches light and shadow, and it can interfere with paint adhesion or a label sitting flat. The right response is not to argue about whether it matters, but to agree in advance which faces are cosmetic and how much dip is acceptable there. That agreement belongs in the RFQ, and this guide ends with it.

The resin you choose changes how hard this fight is. Protolabs rates ABS, polycarbonate and ABS/polycarbonate blends as the most cosmetic-friendly resins, while acetal and PBT are less forgiving, and glass-filled resins and TPE are the most challenging for cosmetics. That ranking is about the whole cosmetic picture — sink, texture, flash — not sink alone, but it is a useful first filter: if your part must have a flawless gloss face, the resin decision and the geometry decision have to be made together, not one after the other.

Read the Mark: Where It Sits Tells You the Cause

The fastest diagnosis in sink-mark troubleshooting costs nothing: turn the part over and look at what sits behind the dip. Sink marks follow mass — the surface tells you where the part is thicker than it should be. Work through the table below before changing any setting, because the location narrows the cause to one or two candidates.

Where the mark appears Usual cause First check
Directly opposite a rib Rib too thick at its base; the rib-wall junction is a pocket of extra material Measure the rib thickness against the nominal wall (see the worked check below)
Directly opposite a boss Solid boss, or a boss wall too thick for the face it stands on Check the boss wall and whether the boss is cored out
Near the gate Packing stopped too early — the gate froze before the thick section was fed Gate size and the hold-time / part-weight test
Across a whole face Wall thickness varies, or a heavy section hides behind the face Map the wall thickness; look for an un-cored thick area
At a wall junction or inside corner Sharp corner concentrates mass and heat where no cooling line can reach Add a radius; step the thickness down gradually
Only on some cavities Cavities are not filling or packing evenly Compare the same feature cavity by cavity
Moves or changes between shots The process itself is unstable — shot size, cushion or material condition varies Stabilise the process first; no setting comparison is valid until the process repeats

Two habits make this reading reliable. First, check the mark under the light your customer will use: a dip that is invisible under flat workshop light can be obvious under a single raking light, and a gloss black face shows a dip that a grained light-grey face hides. Fictiv’s sink-mark guide puts it plainly — glossy surfaces and darker colours make sink marks more pronounced, while textured surfaces and lighter colours help minimise their visibility. Second, judge the part after it has cooled to room temperature and stabilised, not warm off the press: a part straight out of the mold is still shrinking, and a dip judged in the first minutes will look different an hour later. Measure the defect on a settled part, under agreed light, or you will chase a moving target.

The Four Causes, in the Order That Matters

Sink marks are almost never caused by a single variable. They come from four families of causes, and the order in which you address them is the whole point of this guide: design first, mold second, process third, material last. A fix made in the wrong order is not just slower — it can make the next fix impossible, because a process change that masks a geometry problem leaves the geometry in the drawing for the next tool.

1. Part design — decided on paper, cheapest to fix. Most sink marks are designed into the part before any steel is cut. The rules are simple and they are the same in every reputable design guide, because they are physics, not preference. Fictiv’s design guidelines give the standard numbers: make ribs 50% to 60% as thick as the nominal wall, keep rib height to about three times the wall, add 0.5° of draft to each side of the rib, make the bottom of a boss 60% of the nominal wall, and put a fillet of about a quarter of the wall thickness at the rib base. Protomold’s design tips, republished by Design Engineering, give a slightly wider rib range of 40% to 60% and add the boss rule in the same terms: treat the boss wall as a rib and keep it to 40–60% of the wall, or move the boss away from the wall and connect it with a rib of suitable size. Either range leads to the same practice: on a cosmetic face, use 50% and you have margin; above 60% you are building a sink mark into the drawing.

The subtler design cause is the intersection. A rib and a wall can each be within their limits and still create a thick spot where they meet, because the junction adds the two thicknesses together. The same is true of a boss standing on a wall, a clip moulded onto a face, or a sudden step from a thin wall to a thick one. The cure is the same in every case: core out the thick area from the back, thin the feature, add a radius at the root so mass does not pile up at a sharp corner, and step thickness changes down gradually instead of all at once. If you remember one sentence from this section, make it this one: stiffness comes from ribs, not from thick walls.

2. Mold design — gates, cooling, venting. A good part design can still sink if the mold cannot feed and cool the thick section. The gate is the first suspect: a gate that is too small freezes before packing is finished, and a gate placed far from the thick section loses pressure along the flow path, so the section that needs feeding most gets fed least. The gate belongs in or near the thick area whenever the part allows it. Cooling is the second: the thick feature needs a cooling line near it, and where straight lines cannot reach — around a tall boss, behind a side action — the toolmaker may use a bubbler, a conformal channel or a high-conductivity insert such as beryllium copper. Venting is the third and the most often overlooked: trapped air prevents the cavity from packing out fully, and the under-packed region sinks. A sink mark that appears only in one corner of a part, far from the gate, is often a venting problem wearing a sink mark’s clothes.

3. Process — packing, hold time, temperatures. On the press, sink marks are corrected in a fixed order: packing pressure first, then hold time until the gate seals, then melt and mold temperature. Raising pack pressure in small steps feeds more material into the thick section while the gate is still open. Extending hold time keeps feeding until the gate freezes — and no longer: once the gate has sealed, extra hold time feeds nothing, it only lengthens the cycle. Lowering melt temperature reduces how much the resin has to shrink, but only within the resin manufacturer’s recommended range; too cold and you trade a sink mark for a short shot or a weld line. Lowering mold temperature evens cooling, but it does not feed material, so it cannot fix a sink that is really a packing problem. The discipline is to change one variable at a time and to confirm the process is stable first — if shot weight or cushion wanders from cycle to cycle, a sink mark that comes and goes is telling you about the process, not the part.

4. Material — shrinkage is a property, not a setting. Amorphous resins shrink little and evenly; semi-crystalline resins shrink more, and differently along and across the flow. The table below uses shrinkage ranges published in Fictiv’s injection molding specifications and in Protomold’s design guidance — treat them as working ranges for comparison, not as a substitute for the grade-specific data sheet of the resin you actually buy.

Resin family Typical linear shrinkage Sink tendency
ABS 0.4–0.7% Low
Polycarbonate (PC) 0.5–0.7% Low
ABS/PC blend 0.4–0.7% Low
Polypropylene (PP) 1.0–2.5% High
Nylon (PA6, PA66) 1.0–2.5% High
Acetal (POM) 1.0–2.5% High
Glass- or mineral-filled grades Lower than the unfilled base resin Reduced — fillers restrain shrinkage, but check the effect on warpage and surface finish

Two practical consequences follow. First, the same geometry that is sink-free in ABS can sink visibly in PP, because the PP section has roughly three times as much shrinkage to compensate — so a part that changes resin needs its rib and boss rules re-checked, not carried over. Second, changing the base resin is a legitimate fix when the geometry cannot change, as Protolabs notes in its cosmetics guide, but it is a fix with side effects: a filled resin that shrinks less may also warp differently and will never take a high polish the way an unfilled resin does. Colour and finish, by contrast, change only visibility, not the sink itself — a lighter colour and a grained finish hide a shallow dip; they do not remove it.

Worked Check: Is Your Rib the Problem?

Here is the check to run before any meeting about process settings. It takes five minutes with a caliper and it settles the most common argument in sink-mark troubleshooting.

The example — clearly labelled as an illustrative check, not a measurement of any real part. Take an ABS enclosure cover with a nominal wall of 3.0 mm. The drawing shows a stiffening rib on the back of the cosmetic face, drawn 2.4 mm thick. The visible face has a shallow dip directly opposite the rib.

Step 1 — the ratio. Divide the rib by the wall: 2.4 ÷ 3.0 = 80%. The design rule for a cosmetic face is 50–60%. The rib is a third thicker than the top of the range, so the junction behind the face carries far more material than the wall around it. The rib is the prime suspect.

Step 2 — the correction. At 50% of the wall, the rib would be 1.5 mm thick; at the 60% upper limit, 1.8 mm. Either value removes the excess mass at the junction while keeping most of the stiffening effect — stiffness comes mainly from the rib’s height, not its thickness, which is why thinning a rib rarely weakens the part the way a designer fears. If the rib must stay thick for a load the drawing actually states, the alternative is to core the rib out from the back, or to split one thick rib into two thinner ones.

Step 3 — the depth estimate. How deep a dip should you expect? As an order-of-magnitude estimate only — not a prediction of the depth on any real part — multiply the extra thickness behind the face by the resin’s linear shrinkage. The rib junction adds roughly 3 mm of extra material depth behind the face. In ABS at about 0.5% shrinkage, that is 3 × 0.005 = 0.015 mm. In PP at about 1.5%, it is 3 × 0.015 = 0.045 mm — three times as deep, from the same drawing. The estimate does not tell you the exact depth, because real shrinkage depends on the grade, the packing and the cooling; it tells you why the same rib is a non-issue in one resin and a reject in another, and why changing resin without changing the drawing rarely settles the argument.

Step 4 — the decision. If the ratio is above 60% on a cosmetic face, fix the drawing before touching the press: no process setting can feed a junction that was designed to be a heat reservoir. If the ratio is already at 50% and the mark remains, the geometry is not the cause — move on to the gate and packing checks in the next section. If the ratio is between 60% and 50% and the mark is marginal, the finish decision may settle it: a grained texture and a lighter colour can make a 0.02 mm dip disappear, but only after the geometry is inside the rules.

The same check applies to bosses, with the numbers from our threaded insert guide: a boss wall thicker than about 60% of the nominal wall will sink the face it stands on, and a solid boss is worse than a hollow one of the same outside diameter. Hollow the boss, support it with ribs instead of a solid core, and size the boss to the insert — not to the space available.

The Press-Side Fixes — and Their Limits

When the geometry is inside the rules and the mark is still there, the press is the right place to look. Work through the fixes in this order, changing one variable at a time, and stop as soon as the mark is gone — every fix has a limit, and pushing past it creates a different defect.

Fix, in try order What it does When it works Its limit
1. Raise pack pressure in small steps Forces more melt into the thick section while the gate is open The gate is still open and the section is under-packed Too much pressure causes flash, over-packing and molded-in stress; it cannot help if the gate has already frozen
2. Extend hold time to gate seal Keeps feeding until the gate freezes The gate seals late and the section needs more time No effect after the gate seals; extra time only lengthens the cycle
3. Lower melt temperature within the data-sheet range Less shrinkage to compensate Melt temperature is running high Too cold causes short shots, weld lines and poor surface
4. Lower mold temperature / even out cooling Freezes the skin sooner and cools the thick section more evenly A local hot spot is driving the sink Cooling does not feed material — it cannot fix a packing problem
5. Stabilise shot size and cushion Makes the process repeatable so a comparison means something The sink varies from shot to shot If the process will not repeat, no setting change can be judged

The most useful press-side test is the gate-seal check, and it needs no special equipment: mould a series of parts at increasing hold times, weigh each one, and plot the weight. While the gate is still open, longer hold time means a heavier part, because material is still being fed in. When the weight stops rising, the gate has sealed — that hold time is the longest useful one, and any sink mark that remains after it is not a hold-time problem. If the weight never plateaus, the gate may be too large or the material may be back-flowing, and that is a different investigation.

One warning belongs here, because it is the trap this defect sets most often. Protolabs’ cosmetics guide shows the same part moulded three ways: slowing the injection speed to remove gate blush produced an orange-peel surface; raising the speed removed the orange peel but made the sink in the thick areas worse; only redesigning the thick sections out of the part fixed the appearance. Cosmetic problems are cross-coupled — fixing one can worsen another — so a press-side fix that trades a sink mark for flash, a weld line or a blush has not fixed anything. When two defects pull the process in opposite directions, the answer is almost always in the geometry, not in a compromise setting.

When the Press Cannot Fix It

There is a point in every sink-mark investigation where the honest answer is that the tool has to change. Recognising that point early saves the money that gets spent on weeks of process trials. The signs are consistent: the rib and boss ratios are inside the rules, the gate-seal test shows the gate is sealing, pack pressure is already at the point where flash appears, and the mark is still there. At that point the fix is steel, not settings.

The steel fixes, in order of cost, are: core out the thick section from the back so the wall is uniform; thin the rib or hollow the boss; enlarge the gate or move it closer to the thick section so packing reaches it; and add cooling where the thick feature sits — a bubbler, a conformal channel, or a high-conductivity insert where straight lines cannot reach. A texture or a lighter colour can be part of the answer, but with a caveat Protolabs records in the same cosmetics guide: a textured surface can also shadow a mild blemish, because the raised features of the texture cast shadows when light strikes at an angle. Finish hides a shallow dip; it does not remove the cause, and on a face the customer inspects closely it is a weak defence on its own.

One further option exists for parts whose thick sections are structural and cannot be cored out: gas-assisted injection molding. In that process nitrogen is injected into the still-molten core of the thick section, hollowing it from the inside while the gas pressure holds the surface out against the mold wall through cooling — which removes the sink at its source. Mack Molding, the US custom molder, reports that external gas-assist cuts the required molding pressure to 1–2 tons per square inch and roughly halves the clamp tonnage, and that internal gas-assist cuts part weight by 20–30%. It is a real solution for handles, frames and thick structural sections, but it is not a free one: it needs gas injector pins, a sealed gas entry and a second control loop, so it pays only when the section is genuinely thick and the volume justifies the equipment. For most sink-mark problems, the cheaper answer is a thinner rib Before committing to the tooling premium, run the part through the five-question fit test in our gas-assisted injection molding buyer’s guide..

The cost order is the reason to do this work before steel is cut. A design change on paper costs nothing. A process change costs a trial. A steel change after T1 costs a tool modification, a re-trial and a delay. That is why the DFM review matters before you approve a mold: the rib and boss ratios, the gate position and the cooling layout are all visible in the DFM report, and a sink mark found there is fixed with a revised drawing instead of a modified tool.

How to Write the Cosmetic Standard Into Your RFQ

Most sink-mark disputes are not technical disagreements; they are missing agreements. The buyer expected a perfect face, the supplier inspected to a dimensional standard, and nobody wrote down what "acceptable" meant. Put these five lines in the RFQ and the argument never starts:

  1. Classify every face. Mark each surface A (directly visible in use), B (visible at an angle or on close inspection) or C (hidden in assembly). State the SPI finish grade for each face — a gloss A-face and a grained C-face are judged to different standards, and the finish changes how visible a dip is.
  2. Agree how the mark is judged. Name the acceptance method: an approved limit sample showing the worst acceptable dip, or a depth threshold per face class, judged under an agreed light on parts that have cooled and stabilised. A limit sample both sides can hold is worth more than a paragraph of adjectives.
  3. State the resin, grade and colour. Colour changes visibility — dark gloss shows a dip, light texture hides it — and the grade sets the shrinkage the geometry must live with. A resin change after the tool is built re-opens every ratio in this guide.
  4. Require T1 evidence. Ask for the sink check per cavity at T1: photographs of the cosmetic faces, the gate-seal data behind the hold time, and the rib and boss ratios as drawn. A T1 sample without a cosmetic-face record is an incomplete T1.
  5. Agree before steel what happens if sink appears at T1. Write down whether the fix is a process adjustment or a steel change, and who bears the change when the cause is the drawing, the tool or the process. The time to agree that is before the tool is cut, not after the first samples arrive.

What to Send With Your RFQ

A sink-mark-free part starts with a complete RFQ. Send these ten items with your inquiry, and the supplier can quote the cosmetic standard instead of guessing it:

  1. STEP file and 2D drawing, with the nominal wall thickness and the rib and boss thicknesses dimensioned — not just shown.
  2. Face classification (A/B/C) marked on the drawing, with the SPI finish grade for each face.
  3. Resin grade, filler and colour — or the properties the resin must meet, so the supplier can propose a grade and state its shrinkage.
  4. The sink acceptance method: limit sample or depth threshold per face class, and the light it is judged under.
  5. Annual quantity and batch size, so the supplier can judge whether a steel fix or a process fix is the economic answer.
  6. Key tolerances, and which dimensions are cosmetic-critical rather than functionally critical.
  7. Gate position preference, if any — and whether the gate may sit on a cosmetic face.
  8. Any texture or paint the part will carry, since both change what a dip looks like.
  9. The T1 evidence you expect: cosmetic-face photographs per cavity and the gate-seal data.
  10. Delivery region and timing, so the supplier can plan the trial and the shipping.

Send the package through our request-a-quote page — a STEP file, a 2D drawing, the material, quantities, key tolerances, surface finish, delivery region and timing are enough for a first review, and we will confirm the cosmetic standard with you before quoting the tool.

Frequently Asked Questions

Can a sink mark be polished out?

No. A sink mark is a depression in the surface, not a mark on it, so polishing removes material from around the dip and usually makes it more visible, not less. The only cosmetic rescue is a texture or a paint that hides the dip — and that is a concession, not a fix. The fix is geometry, gate or packing, in that order.

Will a thicker wall make my part stronger without causing sink?

Almost never. Thickness is the least efficient way to add stiffness, and it is the most reliable way to add a sink mark: a thick section cools last, shrinks most and pulls the face in. Add ribs instead — thin, tall ribs at 50–60% of the wall give more stiffness per gram than a thick wall, and they cool at nearly the same rate as the wall they stand on. If the part genuinely needs a thick section for a load the drawing states, core it out from the back or consider gas-assist, rather than leaving a solid block.

My supplier says "just increase the pack pressure." When is that the wrong answer?

When the gate has already frozen, or when the rib is 80% of the wall. Pack pressure can only feed a section while the gate is open; once it seals, no pressure setting reaches the thick core. And when the geometry is the cause, higher pressure masks the mark on some shots while adding flash, stress and warpage on others. Ask for the gate-seal test — part weight against hold time — and for the rib-to-wall ratio as drawn. If the weight has plateaued and the ratio is above 60%, the press has nothing left to give, and the drawing or the tool has to change.Your production samples arrive, and the part measures to print — but the visible face has a shallow dip, where a rib sits on the back. The supplier calls it cosmetic. Your customer calls it a reject. A sink mark is the most common cosmetic defect in injection molding, and one of the most misdiagnosed: the fix depends on where the mark sits, and the most expensive mistake is changing the process when the geometry is the problem.

A sink mark is a shallow depression where a thick section — a rib, a boss, or a wall junction — cooled and shrank after the surface had frozen, pulling the skin inward. Read the mark’s location: opposite a rib means the rib is too thick, near the gate means packing stopped too early, across a face means the wall is uneven. Fix in this order — geometry, then mold, then process — because no pack pressure can feed a section whose gate has frozen. A rib over 60% of the wall is the usual culprit; bring it to 50% and the marks disappear.

What a Sink Mark Is — and What It Is Not

When molten plastic fills a mold, it does not freeze all at once. The plastic touching the cold steel wall forms a solid skin within a fraction of a second, while the core of a thick section stays molten for much longer. As that core finally cools, it shrinks — all resins shrink as they cool — and because the skin has already set, the shrinking core has nowhere to take material from. So it pulls the skin inward. The result is a shallow, dish-shaped dip on the surface, always directly above the thick feature underneath.

Three distinctions matter, because each points to a different fix. A sink mark is a surface depression: the skin gave way. A void is the same shrinkage hidden inside the part: the skin was stiff enough to hold its shape — common in rigid resins such as unfilled polycarbonate or acrylic — so the core tore away from itself instead, leaving an internal bubble you may only find by sectioning the part or by X-ray. A sink mark is not a short shot (the cavity never filled, so the part is incomplete) and it is not a weld line (two flow fronts met and left a visible seam). If the surface is complete and the dimensions are right but there is a dip, it is a sink mark.

It is also worth stating plainly what a sink mark is not: a dimensional failure. The part still measures to print. That is exactly why sink marks cause so many arguments between buyers and suppliers. The supplier’s inspection sheet says the part passes; the buyer’s customer sees a dip in the middle of a gloss black cover and sends it back. The defect is cosmetic, but "cosmetic" does not mean unimportant — on a visible face, a sink mark reads as poor quality, it catches light and shadow, and it can interfere with paint adhesion or a label sitting flat. The right response is not to argue about whether it matters, but to agree in advance which faces are cosmetic and how much dip is acceptable there. That agreement belongs in the RFQ, and this guide ends with it.

The resin you choose changes how hard this fight is. Protolabs rates ABS, polycarbonate and ABS/polycarbonate blends as the most cosmetic-friendly resins, while acetal and PBT are less forgiving, and glass-filled resins and TPE are the most challenging for cosmetics. That ranking is about the whole cosmetic picture — sink, texture, flash — not sink alone, but it is a useful first filter: if your part must have a flawless gloss face, the resin decision and the geometry decision have to be made together, not one after the other.

Read the Mark: Where It Sits Tells You the Cause

The fastest diagnosis in sink-mark troubleshooting costs nothing: turn the part over and look at what sits behind the dip. Sink marks follow mass — the surface tells you where the part is thicker than it should be. Work through the table below before changing any setting, because the location narrows the cause to one or two candidates.

Where the mark appears Usual cause First check
Directly opposite a rib Rib too thick at its base; the rib-wall junction is a pocket of extra material Measure the rib thickness against the nominal wall (see the worked check below)
Directly opposite a boss Solid boss, or a boss wall too thick for the face it stands on Check the boss wall and whether the boss is cored out
Near the gate Packing stopped too early — the gate froze before the thick section was fed Gate size and the hold-time / part-weight test
Across a whole face Wall thickness varies, or a heavy section hides behind the face Map the wall thickness; look for an un-cored thick area
At a wall junction or inside corner Sharp corner concentrates mass and heat where no cooling line can reach Add a radius; step the thickness down gradually
Only on some cavities Cavities are not filling or packing evenly Compare the same feature cavity by cavity
Moves or changes between shots The process itself is unstable — shot size, cushion or material condition varies Stabilise the process first; no setting comparison is valid until the process repeats

Two habits make this reading reliable. First, check the mark under the light your customer will use: a dip that is invisible under flat workshop light can be obvious under a single raking light, and a gloss black face shows a dip that a grained light-grey face hides. Fictiv’s sink-mark guide puts it plainly — glossy surfaces and darker colours make sink marks more pronounced, while textured surfaces and lighter colours help minimise their visibility. Second, judge the part after it has cooled to room temperature and stabilised, not warm off the press: a part straight out of the mold is still shrinking, and a dip judged in the first minutes will look different an hour later. Measure the defect on a settled part, under agreed light, or you will chase a moving target.

The Four Causes, in the Order That Matters

Sink marks are almost never caused by a single variable. They come from four families of causes, and the order in which you address them is the whole point of this guide: design first, mold second, process third, material last. A fix made in the wrong order is not just slower — it can make the next fix impossible, because a process change that masks a geometry problem leaves the geometry in the drawing for the next tool.

1. Part design — decided on paper, cheapest to fix. Most sink marks are designed into the part before any steel is cut. The rules are simple and they are the same in every reputable design guide, because they are physics, not preference. Fictiv’s design guidelines give the standard numbers: make ribs 50% to 60% as thick as the nominal wall, keep rib height to about three times the wall, add 0.5° of draft to each side of the rib, make the bottom of a boss 60% of the nominal wall, and put a fillet of about a quarter of the wall thickness at the rib base. Protomold’s design tips, republished by Design Engineering, give a slightly wider rib range of 40% to 60% and add the boss rule in the same terms: treat the boss wall as a rib and keep it to 40–60% of the wall, or move the boss away from the wall and connect it with a rib of suitable size. Either range leads to the same practice: on a cosmetic face, use 50% and you have margin; above 60% you are building a sink mark into the drawing.

The subtler design cause is the intersection. A rib and a wall can each be within their limits and still create a thick spot where they meet, because the junction adds the two thicknesses together. The same is true of a boss standing on a wall, a clip moulded onto a face, or a sudden step from a thin wall to a thick one. The cure is the same in every case: core out the thick area from the back, thin the feature, add a radius at the root so mass does not pile up at a sharp corner, and step thickness changes down gradually instead of all at once. If you remember one sentence from this section, make it this one: stiffness comes from ribs, not from thick walls.

2. Mold design — gates, cooling, venting. A good part design can still sink if the mold cannot feed and cool the thick section. The gate is the first suspect: a gate that is too small freezes before packing is finished, and a gate placed far from the thick section loses pressure along the flow path, so the section that needs feeding most gets fed least. The gate belongs in or near the thick area whenever the part allows it. Cooling is the second: the thick feature needs a cooling line near it, and where straight lines cannot reach — around a tall boss, behind a side action — the toolmaker may use a bubbler, a conformal channel or a high-conductivity insert such as beryllium copper. Venting is the third and the most often overlooked: trapped air prevents the cavity from packing out fully, and the under-packed region sinks. A sink mark that appears only in one corner of a part, far from the gate, is often a venting problem wearing a sink mark’s clothes.

3. Process — packing, hold time, temperatures. On the press, sink marks are corrected in a fixed order: packing pressure first, then hold time until the gate seals, then melt and mold temperature. Raising pack pressure in small steps feeds more material into the thick section while the gate is still open. Extending hold time keeps feeding until the gate freezes — and no longer: once the gate has sealed, extra hold time feeds nothing, it only lengthens the cycle. Lowering melt temperature reduces how much the resin has to shrink, but only within the resin manufacturer’s recommended range; too cold and you trade a sink mark for a short shot or a weld line. Lowering mold temperature evens cooling, but it does not feed material, so it cannot fix a sink that is really a packing problem. The discipline is to change one variable at a time and to confirm the process is stable first — if shot weight or cushion wanders from cycle to cycle, a sink mark that comes and goes is telling you about the process, not the part.

4. Material — shrinkage is a property, not a setting. Amorphous resins shrink little and evenly; semi-crystalline resins shrink more, and differently along and across the flow. The table below uses shrinkage ranges published in Fictiv’s injection molding specifications and in Protomold’s design guidance — treat them as working ranges for comparison, not as a substitute for the grade-specific data sheet of the resin you actually buy.

Resin family Typical linear shrinkage Sink tendency
ABS 0.4–0.7% Low
Polycarbonate (PC) 0.5–0.7% Low
ABS/PC blend 0.4–0.7% Low
Polypropylene (PP) 1.0–2.5% High
Nylon (PA6, PA66) 1.0–2.5% High
Acetal (POM) 1.0–2.5% High
Glass- or mineral-filled grades Lower than the unfilled base resin Reduced — fillers restrain shrinkage, but check the effect on warpage and surface finish

Two practical consequences follow. First, the same geometry that is sink-free in ABS can sink visibly in PP, because the PP section has roughly three times as much shrinkage to compensate — so a part that changes resin needs its rib and boss rules re-checked, not carried over. Second, changing the base resin is a legitimate fix when the geometry cannot change, as Protolabs notes in its cosmetics guide, but it is a fix with side effects: a filled resin that shrinks less may also warp differently and will never take a high polish the way an unfilled resin does. Colour and finish, by contrast, change only visibility, not the sink itself — a lighter colour and a grained finish hide a shallow dip; they do not remove it.

Worked Check: Is Your Rib the Problem?

Here is the check to run before any meeting about process settings. It takes five minutes with a caliper and it settles the most common argument in sink-mark troubleshooting.

The example — clearly labelled as an illustrative check, not a measurement of any real part. Take an ABS enclosure cover with a nominal wall of 3.0 mm. The drawing shows a stiffening rib on the back of the cosmetic face, drawn 2.4 mm thick. The visible face has a shallow dip directly opposite the rib.

Step 1 — the ratio. Divide the rib by the wall: 2.4 ÷ 3.0 = 80%. The design rule for a cosmetic face is 50–60%. The rib is a third thicker than the top of the range, so the junction behind the face carries far more material than the wall around it. The rib is the prime suspect.

Step 2 — the correction. At 50% of the wall, the rib would be 1.5 mm thick; at the 60% upper limit, 1.8 mm. Either value removes the excess mass at the junction while keeping most of the stiffening effect — stiffness comes mainly from the rib’s height, not its thickness, which is why thinning a rib rarely weakens the part the way a designer fears. If the rib must stay thick for a load the drawing actually states, the alternative is to core the rib out from the back, or to split one thick rib into two thinner ones.

Step 3 — the depth estimate. How deep a dip should you expect? As an order-of-magnitude estimate only — not a prediction of the depth on any real part — multiply the extra thickness behind the face by the resin’s linear shrinkage. The rib junction adds roughly 3 mm of extra material depth behind the face. In ABS at about 0.5% shrinkage, that is 3 × 0.005 = 0.015 mm. In PP at about 1.5%, it is 3 × 0.015 = 0.045 mm — three times as deep, from the same drawing. The estimate does not tell you the exact depth, because real shrinkage depends on the grade, the packing and the cooling; it tells you why the same rib is a non-issue in one resin and a reject in another, and why changing resin without changing the drawing rarely settles the argument.

Step 4 — the decision. If the ratio is above 60% on a cosmetic face, fix the drawing before touching the press: no process setting can feed a junction that was designed to be a heat reservoir. If the ratio is already at 50% and the mark remains, the geometry is not the cause — move on to the gate and packing checks in the next section. If the ratio is between 60% and 50% and the mark is marginal, the finish decision may settle it: a grained texture and a lighter colour can make a 0.02 mm dip disappear, but only after the geometry is inside the rules.

The same check applies to bosses, with the numbers from our threaded insert guide: a boss wall thicker than about 60% of the nominal wall will sink the face it stands on, and a solid boss is worse than a hollow one of the same outside diameter. Hollow the boss, support it with ribs instead of a solid core, and size the boss to the insert — not to the space available.

The Press-Side Fixes — and Their Limits

When the geometry is inside the rules and the mark is still there, the press is the right place to look. Work through the fixes in this order, changing one variable at a time, and stop as soon as the mark is gone — every fix has a limit, and pushing past it creates a different defect.

Fix, in try order What it does When it works Its limit
1. Raise pack pressure in small steps Forces more melt into the thick section while the gate is open The gate is still open and the section is under-packed Too much pressure causes flash, over-packing and molded-in stress; it cannot help if the gate has already frozen
2. Extend hold time to gate seal Keeps feeding until the gate freezes The gate seals late and the section needs more time No effect after the gate seals; extra time only lengthens the cycle
3. Lower melt temperature within the data-sheet range Less shrinkage to compensate Melt temperature is running high Too cold causes short shots, weld lines and poor surface
4. Lower mold temperature / even out cooling Freezes the skin sooner and cools the thick section more evenly A local hot spot is driving the sink Cooling does not feed material — it cannot fix a packing problem
5. Stabilise shot size and cushion Makes the process repeatable so a comparison means something The sink varies from shot to shot If the process will not repeat, no setting change can be judged

The most useful press-side test is the gate-seal check, and it needs no special equipment: mould a series of parts at increasing hold times, weigh each one, and plot the weight. While the gate is still open, longer hold time means a heavier part, because material is still being fed in. When the weight stops rising, the gate has sealed — that hold time is the longest useful one, and any sink mark that remains after it is not a hold-time problem. If the weight never plateaus, the gate may be too large or the material may be back-flowing, and that is a different investigation.

One warning belongs here, because it is the trap this defect sets most often. Protolabs’ cosmetics guide shows the same part moulded three ways: slowing the injection speed to remove gate blush produced an orange-peel surface; raising the speed removed the orange peel but made the sink in the thick areas worse; only redesigning the thick sections out of the part fixed the appearance. Cosmetic problems are cross-coupled — fixing one can worsen another — so a press-side fix that trades a sink mark for flash, a weld line or a blush has not fixed anything. When two defects pull the process in opposite directions, the answer is almost always in the geometry, not in a compromise setting.

When the Press Cannot Fix It

There is a point in every sink-mark investigation where the honest answer is that the tool has to change. Recognising that point early saves the money that gets spent on weeks of process trials. The signs are consistent: the rib and boss ratios are inside the rules, the gate-seal test shows the gate is sealing, pack pressure is already at the point where flash appears, and the mark is still there. At that point the fix is steel, not settings.

The steel fixes, in order of cost, are: core out the thick section from the back so the wall is uniform; thin the rib or hollow the boss; enlarge the gate or move it closer to the thick section so packing reaches it; and add cooling where the thick feature sits — a bubbler, a conformal channel, or a high-conductivity insert where straight lines cannot reach. A texture or a lighter colour can be part of the answer, but with a caveat Protolabs records in the same cosmetics guide: a textured surface can also shadow a mild blemish, because the raised features of the texture cast shadows when light strikes at an angle. Finish hides a shallow dip; it does not remove the cause, and on a face the customer inspects closely it is a weak defence on its own.

One further option exists for parts whose thick sections are structural and cannot be cored out: gas-assisted injection molding. In that process nitrogen is injected into the still-molten core of the thick section, hollowing it from the inside while the gas pressure holds the surface out against the mold wall through cooling — which removes the sink at its source. Mack Molding, the US custom molder, reports that external gas-assist cuts the required molding pressure to 1–2 tons per square inch and roughly halves the clamp tonnage, and that internal gas-assist cuts part weight by 20–30%. It is a real solution for handles, frames and thick structural sections, but it is not a free one: it needs gas injector pins, a sealed gas entry and a second control loop, so it pays only when the section is genuinely thick and the volume justifies the equipment. For most sink-mark problems, the cheaper answer is a thinner rib.

The cost order is the reason to do this work before steel is cut. A design change on paper costs nothing. A process change costs a trial. A steel change after T1 costs a tool modification, a re-trial and a delay. That is why the DFM review matters before you approve a mold: the rib and boss ratios, the gate position and the cooling layout are all visible in the DFM report, and a sink mark found there is fixed with a revised drawing instead of a modified tool.

How to Write the Cosmetic Standard Into Your RFQ

Most sink-mark disputes are not technical disagreements; they are missing agreements. The buyer expected a perfect face, the supplier inspected to a dimensional standard, and nobody wrote down what "acceptable" meant. Put these five lines in the RFQ and the argument never starts:

  1. Classify every face. Mark each surface A (directly visible in use), B (visible at an angle or on close inspection) or C (hidden in assembly). State the SPI finish grade for each face — a gloss A-face and a grained C-face are judged to different standards, and the finish changes how visible a dip is.
  2. Agree how the mark is judged. Name the acceptance method: an approved limit sample showing the worst acceptable dip, or a depth threshold per face class, judged under an agreed light on parts that have cooled and stabilised. A limit sample both sides can hold is worth more than a paragraph of adjectives.
  3. State the resin, grade and colour. Colour changes visibility — dark gloss shows a dip, light texture hides it — and the grade sets the shrinkage the geometry must live with. A resin change after the tool is built re-opens every ratio in this guide.
  4. Require T1 evidence. Ask for the sink check per cavity at T1: photographs of the cosmetic faces, the gate-seal data behind the hold time, and the rib and boss ratios as drawn. A T1 sample without a cosmetic-face record is an incomplete T1.
  5. Agree before steel what happens if sink appears at T1. Write down whether the fix is a process adjustment or a steel change, and who bears the change when the cause is the drawing, the tool or the process. The time to agree that is before the tool is cut, not after the first samples arrive.

What to Send With Your RFQ

A sink-mark-free part starts with a complete RFQ. Send these ten items with your inquiry, and the supplier can quote the cosmetic standard instead of guessing it:

  1. STEP file and 2D drawing, with the nominal wall thickness and the rib and boss thicknesses dimensioned — not just shown.
  2. Face classification (A/B/C) marked on the drawing, with the SPI finish grade for each face.
  3. Resin grade, filler and colour — or the properties the resin must meet, so the supplier can propose a grade and state its shrinkage.
  4. The sink acceptance method: limit sample or depth threshold per face class, and the light it is judged under.
  5. Annual quantity and batch size, so the supplier can judge whether a steel fix or a process fix is the economic answer.
  6. Key tolerances, and which dimensions are cosmetic-critical rather than functionally critical.
  7. Gate position preference, if any — and whether the gate may sit on a cosmetic face.
  8. Any texture or paint the part will carry, since both change what a dip looks like.
  9. The T1 evidence you expect: cosmetic-face photographs per cavity and the gate-seal data.
  10. Delivery region and timing, so the supplier can plan the trial and the shipping.

Send the package through our request-a-quote page — a STEP file, a 2D drawing, the material, quantities, key tolerances, surface finish, delivery region and timing are enough for a first review, and we will confirm the cosmetic standard with you before quoting the tool.

Frequently Asked Questions

Can a sink mark be polished out?

No. A sink mark is a depression in the surface, not a mark on it, so polishing removes material from around the dip and usually makes it more visible, not less. The only cosmetic rescue is a texture or a paint that hides the dip — and that is a concession, not a fix. The fix is geometry, gate or packing, in that order.

Will a thicker wall make my part stronger without causing sink?

Almost never. Thickness is the least efficient way to add stiffness, and it is the most reliable way to add a sink mark: a thick section cools last, shrinks most and pulls the face in. Add ribs instead — thin, tall ribs at 50–60% of the wall give more stiffness per gram than a thick wall, and they cool at nearly the same rate as the wall they stand on. If the part genuinely needs a thick section for a load the drawing states, core it out from the back or consider gas-assist, rather than leaving a solid block.

My supplier says "just increase the pack pressure." When is that the wrong answer?

When the gate has already frozen, or when the rib is 80% of the wall. Pack pressure can only feed a section while the gate is open; once it seals, no pressure setting reaches the thick core. And when the geometry is the cause, higher pressure masks the mark on some shots while adding flash, stress and warpage on others. Ask for the gate-seal test — part weight against hold time — and for the rib-to-wall ratio as drawn. If the weight has plateaued and the ratio is above 60%, the press has nothing left to give, and the drawing or the tool has to change.

Facebook
Twitter
LinkedIn

Request A Quote for Your Projects!

Hi there! I’m Jerry, a proud dad and passionate at CKMOLD. With years of hands-on experience in the injection mold and CNC industry, I’ve grown from managing the smallest details on the shop floor to leading international projects with clients across Europe and the U.S.

At CKMOLD, we specialize in precision molds, plastic parts, and CNC solutions that help bring bold product ideas to life. I love solving complex challenges, building long-term partnerships, and pushing the limits of what great manufacturing can do.

Let’s connect, exchange ideas, and grow together—whether you’re looking for a reliable manufacturing partner or just want to talk shop!

Start with the Project Basics

Use this short form for a general inquiry. For a quotation, complete the full RFQ and email any 3D/CAD files separately to jerry@ckmold.com.

Wait, We Have Something Special for You!

Join our mailing list and receive a 10% discount on your next mold or CNC project.