How to Specify Surface Finish for Injection Molded Parts: SPI Grades, Cost, and the RFQ

Flat illustration of three plastic housings showing glossy, satin and matte surface finishes side by side

Your housing arrives and the finish is wrong: one batch looks glossy where the drawing implied matte, another shows every flow line because the mold was polished to a mirror. The drawing said "smooth finish" — and three suppliers read it three different ways. The problem is not the mold. It is that the finish was never actually specified.

The short answer: surface finish for an injection molded part is specified as a standard grade applied to the mold steel — most often an SPI grade from A-1 (mirror polish) to D-3 (coarse blast), or a VDI 3400 texture number — assigned separately to each surface of the part, with enough draft angle for the texture to release. Choose the grade by what each surface must do, not by what looks best in a photograph, and write it into the RFQ per surface: a blanket finish callout is the most expensive way to buy appearance you do not need.

Where Does a Molded Part’s Surface Finish Actually Come From?

Unlike a machined part, which can be polished, blasted or coated after it is made, an injection molded part gets its surface from the mold. Every microscopic ridge, polish stroke or spark crater on the inside of the cavity is copied directly onto the plastic as it fills and packs. The end mills that cut the cavity leave tool marks; if those marks are not removed by stoning, polishing or blasting, they appear on the part.

That is why the finish is a tooling decision, not a post-processing decision. The steel surface is prepared to a defined standard before production starts, and the part comes out finished — which is also why finish affects the tooling quote: preparing the steel takes skilled hand work, and the finer the finish, the more of it there is.

Two consequences follow. First, a finish specification is a manufacturing instruction for the steel, so it must name a standard the toolmaker can work to — a grade, not an adjective. Words such as "smooth," "nice" or "high quality" are not specifications. Second, the finish interacts with the resin, the draft angle and the cosmetic requirements of the part, so it cannot be chosen in isolation.

What Do the SPI Grades A, B, C and D Actually Mean?

The most widely used system is the SPI standard, defined by the Society of the Plastics Industry — the U.S. trade association now known as the Plastics Industry Association (PLASTICS). It classifies mold finishes into twelve grades in four families, defined by the method used to finish the steel. Fictiv, a U.S. manufacturing platform, publishes the full chart:

SPI grade Finish family Finishing method Typical surface roughness (Ra)
A-1 Glossy, super Grade #3, 6000-grit diamond buff 0.012–0.025 µm
A-2 Glossy, high Grade #6, 3000-grit diamond buff 0.025–0.05 µm
A-3 Glossy, normal Grade #15, 1200-grit diamond buff 0.05–0.10 µm
B-1 Semi-glossy, fine 600-grit paper 0.05–0.10 µm
B-2 Semi-glossy, medium 400-grit paper 0.10–0.15 µm
B-3 Semi-glossy, normal 320-grit paper 0.28–0.32 µm
C-1 Matte, fine 600-grit stone 0.35–0.40 µm
C-2 Matte, medium 400-grit stone 0.45–0.55 µm
C-3 Matte, normal 320-grit stone 0.63–0.70 µm
D-1 Textured, satin Dry blast, glass bead #11 0.80–1.00 µm
D-2 Textured, dull Dry blast, #240 aluminum oxide 1.00–2.80 µm
D-3 Textured, rough Dry blast, #24 aluminum oxide 3.20–18.0 µm

Ra, or roughness average, is the average height deviation of the surface profile, measured in micrometres (µm). A smaller Ra means a smoother surface. Note that the SPI grade names a preparation method and a visual family, and the Ra value is the typical result of that method — not a measured guarantee for every part, which is why cosmetic acceptance also needs a reference sample, discussed below.

In practice the four families map to four different jobs:

  • A (diamond polish) is for parts that must look like glass: optical lenses, light pipes, transparent covers and high-gloss piano-black bezels. It is the most expensive family and the least forgiving.
  • B (paper polish) is the workhorse for consumer-facing parts: appliance fronts, electronic housings and automotive interior trim where a soft sheen is wanted without mirror perfection.
  • C (stone finish) is the economical baseline for functional parts: brackets, internal housing walls and industrial parts that are seen but not judged.
  • D (dry blast) is for grip, glare control and hiding minor defects: tool handles, shop equipment and textured consumer grips.

For a hidden surface, an agreed as-machined finish can avoid unnecessary polishing. Identify which tool marks and witness lines are acceptable, and specify any release, sealing or mating requirement separately. As-machined is a supplier condition; it is outside the twelve A–D grades listed above.

How Does the Resin Change What a Finish Looks Like?

The same mold finish produces different results in different resins. A glossy polish that looks excellent in acrylic can look merely average in ABS, and a resin that takes a beautiful matte finish may be a poor choice for a mirror polish. Fictiv publishes a resin-by-finish guide that makes the point concrete:

Resin A-1 to A-3 (glossy) B-1 to B-3 (semi-glossy) C-1 to C-3 (matte) D-1 to D-3 (textured)
ABS Average to good Good to excellent Good to excellent Excellent
Acrylic (PMMA) Excellent Good Good Average
Nylon (PA) Average to good Good to excellent Good to excellent Excellent to good
Polycarbonate (PC) Average to excellent Good to average Good to average Excellent at D-1; not recommended at D-2/D-3
Polypropylene (PP) Not recommended at A-1; average at A-2/A-3 Good to excellent Good to excellent Excellent
Polystyrene (PS) Average to good Excellent Excellent Excellent to good

Use a resin-by-finish chart to shortlist combinations. The appearance of a particular PP or PC grade also depends on fillers, gloss, color and molding conditions. Agree on a plaque or trial part molded in the specified grade and color before funding a mirror polish or coarse texture. The material selection guide for precision injection molding explains the resin choices to settle first.

The resin also affects how visible molding defects are. A high-gloss A-grade surface acts like a magnifying glass: the slightest hesitation line, weld line, gate halo or trace of sink stands out as a visual defect, while a matte or textured surface hides those same marks. Match the finish to the cosmetic standard the part will actually be judged against.

What About VDI 3400 and Mold-Tech Textures?

A drawing may specify a VDI 3400 surface reference. Its designation is distinct from the SPI abrasive method. The table below shows the twelve specimens on BQC’s EDM reference comparator, from VDI 12 through 45. Finer grades also exist. Identify the drawing’s grade and agree on the physical reference and measurement conditions with the toolmaker.

VDI grade Typical surface roughness (Ra) Character
VDI 12 0.40 µm Fine spark matte in this table
VDI 15 0.56 µm Fine matte
VDI 18 0.80 µm Satin matte
VDI 21 1.12 µm Light matte
VDI 24 1.60 µm Medium matte
VDI 27 2.24 µm Medium matte
VDI 30 3.15 µm Coarse matte
VDI 33 4.50 µm Coarse matte
VDI 36 6.30 µm Heavy matte
VDI 39 9.00 µm Heavy texture
VDI 42 12.50 µm Very heavy texture
VDI 45 18.00 µm Coarse texture in this table

Surfaces produced by different methods can have similar average roughness but different gloss and appearance. Record a VDI callout as supplied and approve an actual reference. Agree any alternative in writing before machining or texturing the steel.

For a decorative grain, specify the pattern supplier, pattern code, depth, direction and draw direction. A leather or stipple name alone does not identify a depth. Ask the texture supplier to assess the draft on the actual geometry before approving the pattern.

Why Does Texture Decide the Draft Angle?

Draft angle is the taper on a molded wall that lets the part slide out of the steel. Texture and draft are mechanically inseparable: when molten plastic packs into the microscopic valleys of a textured cavity, the part cannot slide out unless the wall tapers away fast enough for the plastic peaks to clear the steel peaks without shearing. The deeper the texture, the more draft the wall needs.

The following ranges are preliminary screening figures quoted in the original surface finish and draft reference. Obtain the toolmaker’s and texture supplier’s approval for the actual grade, wall depth and direction of draw.

Finish Draft range for initial review
SPI A-1 / A-2 / A-3 (mirror polish) 1.0°–2.0° or more
SPI B-1 / B-2 / B-3 (paper polish) 1.0°–1.5°
SPI C-1 / C-2 / C-3 (stone finish) 1.0°–1.5°
SPI D-1 / D-2 / D-3 (dry blast) 1.5°–3.0° or more, increasing with blast depth
VDI 3400, VDI 18–30 1.5°–3.0° or more
Chemical or laser grain (leather, stipple) 3.0°–5.0° or more

Ask for the supplier’s release allowance for the selected texture and resin. Measure local draft normal to the actual pull direction, including areas near shutoffs and side actions. If the available angle is too small, consider changing the grain, moving the texture boundary or revising the wall before cutting steel.

On a deep smooth core, part shrinkage and restricted air entry can make ejection difficult. Review draw direction, venting, draft and ejection support before changing the surface. SPI B-3 is a 320-grit paper finish; a dry blast is a different preparation. Describe the process actually intended and approve a sample. See Fictiv’s SPI preparation chart and Eastman’s resin-specific mold design guide.

How Does Surface Finish Change the Tool Cost?

Finish costs tooling money in three ways, and the quote has to carry all three:

Cost driver What happens Cheapest Most expensive
Polishing labour Hand stoning and buffing through progressive grits by a specialist polisher As-machined or stone finish Diamond buffing to A-1/A-2
Tool steel grade High polish needs clean, hardenable steel without inclusions Standard pre-hardened steel for B/C finishes Premium vacuum-degassed or ESR stainless (such as 420 ESR / S136) or pre-hardened NAK80 for A grades
Texture work Blasting, EDM, chemical etching or laser texturing, plus reference plaques Dry blast D-1 Deep chemical grain or laser texture

Fictiv states the general rule plainly: finishes that take longer to produce cost more, and finishes that use more expensive abrasives or more complex processes also cost more. The Plastics Technology Alliance adds the detail that matters most: achieving a distortion-free A-1 or A-2 finish requires premium steel, because standard P20 steel can contain microscopic inclusions that cause "orange peel" pitting during diamond buffing — and every square inch must be hand-stoned through progressive grits.

The economical default is a stone finish in the C family on non-cosmetic surfaces, with a finer grade only where the eye actually lands. That is also why finish should be assigned per surface, not per part. One part can carry A-3 on its front face, B-2 on its mating edges and C-2 on its internal ribs — and the quote will reflect exactly that, instead of pricing the whole tool to the finest grade on it.

How Should You Write the Finish into Your RFQ?

A finish specification that gets comparable quotes has six elements. The table below is the checklist to send with the drawing:

# Check Why it matters
1 Finish assigned per surface, not per part The supplier prices the hard work where it is, not everywhere
2 Standard and grade named (e.g. SPI B-2, VDI 27) A grade is quotable; an adjective is a guess
3 Cosmetic surfaces classified (A = visible, B = mating, C = hidden) Appearance standards apply where the eye lands
4 Draft verified against texture depth in CAD Texture without draft drags, scuffs or sticks
5 Gate, ejector and parting-line locations marked Finish cannot hide a gate scar on a Class A face
6 Reference sample or plaque agreed (SPI/VDI plaque, signed boundary sample) Buyer and supplier judge the same standard under the same light

Three habits make the specification work in practice. First, map the finish by surface zone on the drawing — a colour-coded CAD screenshot assigning, for example, VDI 27 on the exterior Class A housing, SPI B-3 on mating Class B edges and SPI C-2 on internal Class C ribs and cores. Second, agree the cosmetic standard before production: both your incoming-quality team and the molder should hold matching physical SPI or VDI reference plaques and evaluate parts under standardised lighting, such as D65 daylight in a light booth. Third, hold texture release until after T1 dimensional sign-off: run T1 sampling on smooth, un-textured steel — for example, paper-finished to SPI B-3 or stoned to SPI C-1 — and authorise chemical or laser texturing in writing only after the dimensions are approved. Repairing a mold after etching leaves a permanent patch mark, because hand re-etching a welded spot rarely blends with the surrounding grain; repairing smooth steel is routine. Smooth T1 parts also expose flow lines, jetting and gas marks that texture would hide, so the molder can correct venting and gate speed before the evidence is covered up.

Tolerances interact with finish as well: a tight tolerance on a textured surface is harder to hold than the same tolerance on a polished one, because the texture itself is a surface variation. If your drawing carries tight tolerances, our guide to injection molding tolerances explains which features justify them and what they cost. And if the DFM review has not yet settled wall thickness, draft and gate positions, our guide to reviewing a DFM report shows what to check before steel is cut — finish is one of the items that should be agreed at that stage, not after.

A Worked Example: Choosing the Finish for a Housing

Consider a hand-held device housing, roughly the size of a paperback book, molded in ABS. The front face is the product’s face to the user; the sides are gripped; the inside holds ribs, bosses and a battery compartment nobody sees.

A reasonable specification, following the logic above, would be: SPI B-1 on the front face, for a fine semi-gloss that looks like a quality consumer product without the cost and defect visibility of a mirror polish; SPI D-1 satin blast on the grip sides, for a non-slip, fingerprint-hiding surface; and SPI C-2 on all internal ribs, bosses and the battery compartment, where a stone finish is the economical baseline. The drawing would mark the front face as Class A, the sides as Class B, and the interior as Class C, with 1.0° draft on the front, 2.0° on the textured sides, and the gate placed on the rear face so no gate scar lands on the Class A surface. Specifying SPI A-2 on every surface instead would buy premium steel and diamond polishing for the battery compartment, and would make every flow line on the front face a visible defect — while specifying "smooth finish" with no grade would leave each supplier to choose, so the quotes would describe three different tools. Neither mistake is a molding failure. Both are specification failures, and both are avoidable before the RFQ goes out.

Frequently Asked Questions

Can the finish be changed after the mold is built?

A toolmaker can assess a finer polish or a deeper texture against the steel allowance, draw direction and mating dimensions. Removing an existing texture removes steel; the resulting change differs between a cavity surface and a core. Ask for a stock-removal and repair plan, identify shutoffs and critical fits, and approve a new sample before authorizing rework.

Who supplies the reference plaque?

Either side can, but both sides must hold the same one. SPI and VDI reference plaques are sold as standard sets; agree in the RFQ which set governs, and keep one plaque with your incoming-quality team and one with the molder. A signed boundary sample — an approved part kept as the visual standard — serves the same purpose for a specific product, and is often the more practical choice once production is running.

What to Send With Your RFQ

Send the 3D CAD file (STEP), a 2D drawing with the finish grade marked per surface, the cosmetic surface classification, the target resin grade, expected quantities, and the draft angles as designed. Add the gate and ejector restrictions for the cosmetic faces, and say whether you will supply a reference plaque or expect the supplier to hold one. That package lets a molder quote the finish work once, accurately — instead of pricing the risk of a drawing that asks for "smooth" and means three different things.

Request a quote for your injection molded parts with your drawing and finish requirements, and we will review the finish plan with the DFM before quoting tooling. Our production injection molding service covers repeat production once the finish and the samples are approved.

Facebook
Twitter
LinkedIn

Request A Quote for Your Projects!

Hi there! I’m Jerry, a proud dad and passionate at CKMOLD. With years of hands-on experience in the injection mold and CNC industry, I’ve grown from managing the smallest details on the shop floor to leading international projects with clients across Europe and the U.S.

At CKMOLD, we specialize in precision molds, plastic parts, and CNC solutions that help bring bold product ideas to life. I love solving complex challenges, building long-term partnerships, and pushing the limits of what great manufacturing can do.

Let’s connect, exchange ideas, and grow together—whether you’re looking for a reliable manufacturing partner or just want to talk shop!

Start with the Project Basics

Use this short form for a general inquiry. For a quotation, complete the full RFQ and email any 3D/CAD files separately to jerry@ckmold.com.

Wait, We Have Something Special for You!

Join our mailing list and receive a 10% discount on your next mold or CNC project.